Low-alloy steels Flux cored wire E81T1-B2C Alurinmorin nkan na
KỌMPUTA kemikali
ALOY(wt%) | C | Mn | Si | Cr | V | Mo | P | S |
GB/T OFIN | 0.05-0.12 | 1.25 | 0.80 | 1.00-1.50 | - | 0.40-0.65 | 0.03 | 0.03 |
Aws ofin | 0.05-0.12 | 1.25 | 0.80 | 1.00-1.50 | - | 0.40-0.65 | 0.03 | 0.03 |
APEERE IYE | 0.052 | 0.88 | 0.28 | 1.12 | 0.105 | 0.46 | 0.009 | 0.005 |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | IMAPACT IYE J/℃ | ÌGBÀGBÀ(%) | Itọju igbona °Cxh | |||||
GB/T OFIN | 470 | 550-690 | - | 17 | 730*2 | |||||
Aws ofin | 470 | 550-690 | - | 19 | 730*2 | |||||
APEERE IYE | 560 | 640 | 50 / Deede otutu | 23 | 730*2 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 1.2 | ||||
Folti | 24-35 | ||||
Amp | 160-320 | ||||
Gigun itẹsiwaju gbigbe (mm) | 15-20 | ||||
Ṣiṣan gaasi (l/min) | 15-25 |
Awọn aaki jẹ rirọ ati iduroṣinṣin, kere si asesejade, lẹwa lara.
Ti o dara slag yiyọ, kere soot.
Pẹlu o tayọ alurinmorin ilana iṣẹ.
-
Zenhai Refining 1 milionu toonu / odun ethylene ise agbese
-
Awọn ohun elo alurinmorin fun awọn ọkọ ayọkẹlẹ iṣinipopada
-
JU2000E jack-soke liluho
KỌMPUTA kemikali
ALOY(wt%) | C | Mn | Si | Cr | V | Mo | P | S |
GB/T OFIN | 0.05-0.12 | 1.25 | 0.80 | 1.00-1.50 | - | 0.40-0.65 | 0.03 | 0.03 |
Aws ofin | 0.05-0.12 | 1.25 | 0.80 | 1.00-1.50 | - | 0.40-0.65 | 0.03 | 0.03 |
APEERE IYE | 0.052 | 0.88 | 0.28 | 1.12 | 0.105 | 0.46 | 0.009 | 0.005 |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | IMAPACT IYE J/℃ | ÌGBÀGBÀ(%) | Itọju igbona °Cxh | |||||
GB/T OFIN | 470 | 550-690 | - | 17 | 730*2 | |||||
Aws ofin | 470 | 550-690 | - | 19 | 730*2 | |||||
APEERE IYE | 560 | 640 | 50 / Deede otutu | 23 | 730*2 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 1.2 | ||||
Folti | 24-35 | ||||
Amp | 160-320 | ||||
Gigun itẹsiwaju gbigbe (mm) | 15-20 | ||||
Ṣiṣan gaasi (l/min) | 15-25 |