Low-alloy steels Afowoyi elekiturodu E7016-A1 Soldering awọn ẹya ẹrọ
KỌMPUTA kemikali
ALOY(wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Omiiran |
GB/T OFIN | 0.065 | 0.35 | 0.65 | 0.015 | 0.01 | 0.03 | 0.04 | 0.5 | - |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | Ilọsiwaju(%) | IMAPACT IYE J/℃ | Itọju ooru °C * h | |||||
GB/T OFIN | 460 | 560 | 27 | 130 / Deede otutu | 620*1 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 3.2*350 | 4.0 * 400 | 5.0 * 400 | ||||
ELECTRICITY (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |
Ọpa alurinmorin ọwọ iru potasiomu kekere, fifi 0.5% Mo, mu agbara weld dara ati resistance ipata
Iduroṣinṣin arc, asesejade ti o kere si, mimu ti o dara, yiyọ slag rọrun
X-Ray išẹ jẹ o tayọ.
-
Sino-Russian iwaju ila-oorun
Harbin ina mẹta ẹnu-bode CMT
-
Awọn ohun elo alurinmorin fun awọn apoti
KỌMPUTA kemikali
ALOY(wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Omiiran |
GB/T OFIN | 0.065 | 0.35 | 0.65 | 0.015 | 0.01 | 0.03 | 0.04 | 0.5 | - |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | Ilọsiwaju(%) | IMAPACT IYE J/℃ | Itọju ooru °C * h | |||||
GB/T OFIN | 460 | 560 | 27 | 130 / Deede otutu | 620*1 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 3.2*350 | 4.0 * 400 | 5.0 * 400 | ||||
ELECTRICITY (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |