Kekere-alloy steels Afowoyi elekiturodu E7018-B2L irin Apapo makings
Iron lulú kekere hydrogen potasiomu iru ọwọ alurinmorin opa, idurosinsin aaki
Asesejade ti o kere si, mimu ti o dara, rọrun lati yọ iṣẹ slag X-Ray kuro
Awọn ohun-ini ẹrọ iduroṣinṣin, lile ipa ti o ga ni a le ṣetọju labẹ awọn ipo itọju ooru
KỌMPUTA kemikali
ALOY(wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Omiiran |
GB/T OFIN | 0.04 | 0.35 | 0.8 | 0.013 | 0.01 | 0.018 | 1.28 | 0.51 | - |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | Ilọsiwaju(%) | IMAPACT IYE J/℃ | Itọju ooru °C * h | |||||
GB/T OFIN | 455 | 560 | 23 | 175 / Deede otutu | 690*1 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 3.2*350 | 4.0 * 400 | 5.0 * 400 | ||||
ELECTRICITY (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |
-
Sino-Russian iwaju ila-oorun
Haiyang iparun agbara ọgbin
-
400,000 toonu irin ti ngbe
KỌMPUTA kemikali
ALOY(wt%) | C | Si | Mn | P | S | Ni | Cr | Mo | Omiiran |
GB/T OFIN | 0.04 | 0.35 | 0.8 | 0.013 | 0.01 | 0.018 | 1.28 | 0.51 | - |
Ohun-ini ẹrọ:
ONÍNÌYÀN | AGBARA YIELD(MPa) | AGBARA Ifaagun (MPa) | Ilọsiwaju(%) | IMAPACT IYE J/℃ | Itọju ooru °C * h | |||||
GB/T OFIN | 455 | 560 | 23 | 175 / Deede otutu | 690*1 |
Niyanju welding PARAMETER:
DIAMETERS PIPICATIONS(mm) | 3.2*350 | 4.0 * 400 | 5.0 * 400 | ||||
ELECTRICITY (Amp) | H/W | 90-130 | 140-190 | 190-240 | |||
O/W | 80-120 | 120-160 | - |