Ninu awọn iṣẹ alurinmorin ti awọn ọkọ oju omi, awọn afara, awọn ẹya irin ati awọn ile-iṣẹ miiran, igbagbogbo awọn welds igun-ọtun gun gun, ati alurinmorin adaṣe jẹ lilo pupọ julọ, pẹlu awọn kẹkẹ alurinmorin, awọn apa alurinmorin laifọwọyi ati awọn ọna alurinmorin olona-electrode daradara siwaju sii. Fun T-row multi-electrode alurinmorin, ile-iṣẹ wa ṣe ifilọlẹ GFL-70C iron powder type flux cored wire with GCL-11G metal powder type welding wire, eyi ti o ti gba nipasẹ awọn onibara siwaju ati siwaju sii. Ọna apapo alurinmorin yii ni iyara alurinmorin giga, alakoko sooro zinc ti o dara julọ, ati iṣelọpọ ileke weld ẹlẹwa. Iṣe ṣiṣe ifisilẹ ti waya iwaju GCL-11G jẹ giga bi 97%, nipataki nitori iye irin kikun, ati okun ẹhin GFL-70C ṣe idaniloju dida ti ileke weld, ati iyara alurinmorin le de ọdọ 1000-1400mm /min. O dara julọ fun alurinmorin alapin ati alurinmorin fillet alapin ti ọpọlọpọ awọn ẹya bii awọn ọkọ oju omi, awọn afara, ẹrọ, awọn ọkọ ati awọn ẹya irin.
Olona-electrode T-kana ga-iyara ati lilo daradara alurinmorin
Irisi ti weld slag yiyọ
Ṣaaju ki o to deslagging
Lẹhin ti deslagging
Ẹya ti o tobi julọ ti ọna alurinmorin yii jẹ ṣiṣe giga rẹ, alurinmorin elekitirodu pupọ ni akoko kanna, ati pe ko si iwulo lati ṣe aibalẹ nipa kikọlu ti polarity ati aaye oofa. Ẹgbẹ kọọkan ti fillet welds ni awọn eto meji ti awọn ògùṣọ alurinmorin, ati ẹgbẹ kọọkan ni awọn okun iwaju ati awọn onirin ẹhin. Ni iwaju waya ni o ni dara porosity resistance ati ki o Sin bi kan ti o tobi iye ti kikun irin. Awọn ru waya nikan nilo lati rii daju wipe awọn weld ileke ti wa ni akoso alapin, aṣọ ati ki o mọ. Awọn abuda ti o wa tẹlẹ ti irin lulú iru ṣiṣan okun waya, bi okun ẹhin ti apapo yii, le kan pade awọn ibeere ti apẹrẹ ti o baamu ati irisi rẹ. Igun ògùṣọ alurinmorin ati atunṣe ijinna ti ọna alurinmorin yii ni a fihan ni aworan ni isalẹ:
Arabara iyara fillet alurinmorin:
Akiyesi: Ṣatunṣe aaye laarin awọn okun iwaju ati ẹhin ni ibamu si ooru gangan ti adagun didà lakoko alurinmorin
Yi alurinmorin ọna le gba awọn ti o fẹ alurinmorin ireti nipa Siṣàtúnṣe iwọn orisirisi alurinmorin sile. Nipa Siṣàtúnṣe iwọn alurinmorin lọwọlọwọ, foliteji, alurinmorin iyara, alurinmorin ijinna, ati be be lo, o yatọ si alurinmorin titobi titobi le ṣee gba.
Apapo iyara fillet alurinmorin ti o ga pupọ 1
GCL-11G (elekiturodu to ti ni ilọsiwaju)/GFL-70C (elekiturodu iwaju) 1.4mm:
Lọwọlọwọ ati foliteji | iyara alurinmorin mm/min | Solder ẹsẹ ipari |
aṣáájú-ọnà 360A/32V Tẹle-soke kilasi 360A/38V Electrode aaye 25MM | 800 | 9-10 |
1000 | 7-8 |
ẹsẹ ipari | 9.0 | ẹsẹ ipari | 7.0 | |
Iyipada | 0.4 | Iyipada | 0.8 | |
Ilaluja | 2.0 | Ilaluja | 2.2 |
Apapo iyara fillet alurinmorin ti o ga pupọ 2
GCL-11G (elekiturodu to ti ni ilọsiwaju)/GFL-70C (elekiturodu iwaju) 1.6mm:
Lọwọlọwọ ati foliteji | iyara alurinmorin mm/min | Solder ẹsẹ ipari |
aṣáájú-ọnà 360A/32V Tẹle-soke kilasi 360A/38V Electrode aaye 25MM | 1000 | 8-9 |
1200 | 7-8 |
Iwari ilaluja
ẹsẹ ipari | 8.0 |
| ẹsẹ ipari | 7.0 |
Iyipada | 0 | Iyipada | 0.3 | |
Ilaluja | 2.4 | Ilaluja | 2.7 |
GCL-11G + GFL-70C iṣeduro ipo alurinmorin
ẹka alurinmorin | Sipesifikesonu mm | alurinmorin sipesifikesonu | iyara alurinmorin mm/min | Solder ẹsẹ iwọn mm | Akiyesi | |
Siliki iwaju | Siliki sẹhin | |||||
apapo | 1.4 | 350-400A 32-36V | 320-380A 36-38V | 700- 1000 | 5-8 | Waya iwaju jẹ GCL-11G, ti a lo fun kikun, lọwọlọwọ giga, foliteji kekere; awọn ru waya ni GFL-70C, ga foliteji, kekere lọwọlọwọ |
1.6 | 360-420A 36-38V | 320-400A 36-38V | 1000- 14000 | 5-8 |
Omiiran: igun alurinmorin 9-12mm le ṣee ṣe nipasẹ ṣiṣatunṣe igun ògùṣọ alurinmorin kan pato ati iyara alurinmorin. Weld ileke bi han ni isalẹ:
12mm tobi alurinmorin igun
Fun ọna alurinmorin yii, jọwọ tun tẹle awọn iṣeduro alurinmorin wọnyi ati awọn iṣọra
1. Ṣe mimọ awọn idoti oju-ilẹ, ipata, awọn abawọn epo, ati awọn iṣẹku oxidation, bibẹẹkọ o le fa awọn pores tabi awọn abawọn bii mimu ti ko dara.
2. Awọn akoonu inu omi ti o pọju yoo ni ipa lori didara alurinmorin ati ki o fa awọn pores. Ti ọriniinitutu ba ga, itusilẹ to dara yẹ ki o ṣe ṣaaju alurinmorin, ati pe o yẹ ki o yago fun alurinmorin alẹ kan ni apa kan.
3. Awọn sisanra ti awọn kikun fiimu ti wa ni gbogbo dari ni 15-35um. Ti sisanra fiimu naa ba nipọn pupọ, yoo fa awọn pores ni rọọrun, ati pe o nilo lati didan ti o ba jẹ dandan.
4. Oṣuwọn ṣiṣan gaasi ti wa ni iṣakoso ni 20-25l / min, elongation gbẹ ti wa ni iṣakoso ni iwọn 20 ~ 25mm, ati iyara afẹfẹ kọja 2m / s, ati pe o nilo ibugbe pataki.
5. Nigbati a ba dapọ alurinmorin:
(1) Ni iwaju waya GCL-11G alurinmorin agbara nronu yan awọn ri to jia, ati awọn ru waya GFL-70C alurinmorin nronu yan awọn mojuto jia;
(2) Nigbati alurinmorin fillet welds, kọọkan ẹgbẹ ti quadrupoles ti wa ni ti gbe jade ni ona kan ti nkọju si kọọkan miiran pẹlu iwaju ati ki o ru onirin.